Solder Paste Stencil Design for Optimal QFN Reliability



Solder Paste Stencil Design for Optimal QFN Reliability
In this study, the volume of solder used in assembly of QFNs was varied to investigate the relationship between standoff height and thermal cycle life.

DOWNLOAD
Authored By:
B. Gumpert
Lockheed Martin, Ocala, FL USA

Summary

The use of bottom terminated components (BTC) has become widespread, specifically the use of Quad Flat No-lead (QFN) packages. The small outline and low height of this package type, improved electrical and thermal performance relative to older packaging technology, and low cost make the QFN/BTC attractive for many applications.

Over the past 15 years, the implementation of the QFN/BTC package has garnered a great amount of attention due to the assembly and inspection process challenges associated with the package. The difference in solder application parameters between the center pad and the perimeter pads complicates stencil design, and must be given special attention to balance the dissimilar requirements.

The lack of leads on the QFN/BTC package and the low standoff height result in significantly less compliance relative to other package types, making the QFN/BTC package more susceptible to CTE mismatch issues. Careful assembly of QFNs and proper printed circuit board (PCB) design can result in acceptable reliability depending on the overall design. One area that has not been well addressed, however, is the impact of die to package size ratio, and how this factor should be considered in circuit card assembly. IPC-7093 mentions the inverse relationship between relative die size and reliability, and Syed and Kang found the relationship to be non-linear, yet die size is seldom noted in component datasheets, and vendor recommendations do not include this ratio as a factor in assembly.

In this study, the volume of solder used in assembly of two QFN/BTC packages will be varied to investigate the relationship between standoff height and thermal cycle life, and to determine acceptable process limits with respect to first-pass yields. The QFNs selected have dissimilar die to package size ratios to assess the impact of this factor on the process window. Solder joint defect levels and thermal cycle results will indicate the ability to adjust manufacturing parameters to achieve a balance between the two objectives of process yield and reliability. The results will define a process window that provides the optimal installation of these packages.

Conclusions

Two QFN/BTC packages were installed onto representative circuit cards using a variety of solder paste applications. Many of the standard guidelines for QFN/BTC application and soldering were followed, with only the solder paste volume adjusted to control the resulting solder joint height and geometry. Actual solder joint height for this assembly was shown to correlate well to expected solder joint height according to the stencil design.

In general, an increase in the amount of solder paste used resulted in an increase in the amount of voiding. This is expected, as the pathways for volatiles to escape are reduced and the overall amount of volatiles is increased as the total solder volume increases. Voiding was low in general, with few instances of voiding exceeding 25% of the soldered area.

Thus far, the failure rates for the various solder joint configurations (height) are not as predicted by the simulation software. Of particular note is the inconsistency of the solder joints on the QFN68 packages at increased solder joint heights. The joints seen in the Figure 8 above make electrical connection, but may represent weak joints that are likely to fail relatively early. This joint variation in the previous testing could have skewed the simulation baseline, and therefore the current prediction, which likely assumes that every joint is exactly the same within the programmed parameters.

Another potential impact that could be impacting thermal cycle survivability is the slight change in the solder joint shape at the toe fillet. The solder stencil was adjusted to vary the amount of solder paste applied at the perimeter pins, resulting in solder joints that had very similar geometry, but which were not exactly the same. The slightly larger solder joints on the locations with a shorter solder joint height could improve the thermal cycle survivability. The simulation software did not allow the size or shape of the toe fillet to be adjusted.

Until more failure data is collected, specific conclusions cannot be substantiated, but the observations and results so far indicate that center pad size (and presumably die to package ratio) should not be ignored when implementing QFNs. There were clear differences in the results between the two packages used in this study. Components with a small center pad are relatively robust not only in thermal cycling, but also with respect to yield and consistency in the manufacturing process.

Components with a large center pad require more attention, as they have a smaller process window for optimal solder joints, and have reduced reliability. Initial results indicate that such a component is best installed with 50% or more in solder paste reduction on the center pad, but more failure data is required to determine the ideal stencil design.

Initially Published in the IPC Proceedings

Comments

Jul 15, 2020

It appears that your concern is predominately the amount of the paste used. With QFN/BTC the mass is more a liability since it will limit the ductility of the post reflowed joint. The Intermetallic layer will also determine the joint survivability post reflow.Newer paste blends have been designed to be more ductile, which is what you are looking for. Key also is what the BTCs are plated with on the soldered/tinned terminations. SAC is very brittle post reflow. SAC will also continue to grow the Intermetallic layer causing the joint to be more brittle as time goes on post reflow. The large center pad is best handled by a window pane print pattern with at least one cross-road on the stencil allowing out-gassing routes for the flux and carriers. Additionally sphere size needs to be considered since the spacing under the QFN/BTC.

Ike Sedberry, ISEDS
Submit A Comment
Comments are reviewed prior to posting. You must include your full name to have your comments posted. We will not post your email address.

Your Name


Your Company
Your E-mail


Your Country
Your Comments



Free Newsletter Subscription
Circuitnet is built for professionals who bear the responsibility of looking ahead, imagining the future, and preparing for it.

Insert Your Email Address

Sponsor
Uyemura
RAIG Minimizes Corrosion, Allows Higher Gold on ENEPIG
Paper describes a mixed reaction RAIG electrolyte that minimizes galvanic corrosion and allows higher ENEPIG gold thicknesses, enabling robust designs and world-class quality on target with minimal variation.
Uyemura
Affordable Profiling