circuitnet
Sponsor
Indium Corporation
High-Reliability for Low-Temp Processes
Durafuse® LT low-temp, high-rel solder paste is bismuth-free, reduces warpage in large BGAs, enhances thermal cycling, drop shock reliability and reduces energy use up to 15%.
Indium Corporation
Openair Plasma for Semiconductor Manufacturing
Sponsor
AI Technology, Inc.
Corrosion, UV Protection for Power Transmission
Moisture, corrosive gas, oxidation & UV blocking prop-erties. FLUOROSEAL® conformal coating for electrical contacts & ceramic insulator protection.
AI Technology, Inc.

Should Apertures be Home Plate or Inverted Home Plate?



Should Apertures be Home Plate or Inverted Home Plate?
Should stencil the aperture be home plate or inverted home plate? You know the performance difference between the two types. Which one is better? Jim Hall and Phil Zarrow, The Assembly Brothers, discuss this question and share their own insights.
Board Talk
Board Talk is presented by Phil Zarrow and Jim Hall of ITM Consulting.
Process Troubleshooting, Failure Analysis, Process Audits, Process Set-up
CEM Selection/Qualification, SMT Training/Seminars, Legal Disputes
Phil Zarrow
Phil Zarrow
With over 50 years experience in PCB assembly, Phil is one of the leading experts in SMT process failure analysis. He has vast experience in SMT equipment, materials and processes.
Jim Hall
Jim Hall
A Lean Six-Sigma Master Blackbelt, Jim has a wealth of knowledge in soldering, thermal technology, equipment and process basics. He is a pioneer in the science of reflow.

Transcript

Phil
And welcome to Board Talk with Jim Hall and Phil Zarrow of ITM Consulting, the Assembly Brothers. And today we are coming to you from the ITM pub, which is located near the base of Mount Rialto so nobody gets hurt.

We're here to talk about electronic assembly, materials, equipment, components, practices, procedures, secret decoder rings and many other things. Jim, what is our question du jour?

Jim
The question come from S.B. regarding home plate stencil apertures. Should the aperture be home plate or inverted home plate?

You know the performance difference between the two types. Which one is better?

Well perhaps, Phil, we should define home plate to make sure we all know what we are talking about, an aperture for a rectangular pad, which is not rectangular, but in fact looks like a home plate, it is five-sided, two right angles, and then a pointy side on the other part.

A traditional home plate had these apertures oriented so that the pointy section pointed towards the center of the component.

They were developed a long time ago to minimize solder beading or mid-chip solder balls.

Phil
Particularly on ceramic capacitors because they had the metal end caps and the idea by narrowing down to that point, there was less propensity, less solder, to be squeezed underneath the center of the component to form that so-called mid-chip solder ball.

It has been pretty traditional as well. But back to the question Jim.

Jim
Right, and that was developed when capacitors were larger, 12060805.  It is probably applicable down to 0603, maybe 0402s.

But historically as we got to the ultra miniature parts, 0402 may fit this but definitely 0201s, mid-chip solder balling became the least of our problems, and tombstoning became a much bigger issue.

And that is where some people have developed what they call inverted, or reversed, home plate, where they rotate that 180 degrees, so that the pointy part of the aperture is not under the component, but is pointing away from the component.

The strategy here was that by minimizing the amount of paste on the outer part of the pad, not underneath the component, when it started to melt it would take time for the solder to flow out from under the part and would and then wet up the vertical end of the chip component. That would minimize the possibility that you would get surface tension forces out of balance, which is the mechanism that creates tombstones.

And some people feel that was very successful, other people were not too excited about that. Obviously when you get to 0201s tombstoning is a huge problem and there are many different strategies, starting with proper pad design and modified paste, and finally shoulder profile developed by Dr. Lee of Indium.

Once you get to slow down the heating right at the melting point to minimize the possibility that the surface tension forces get out of balance and tip the component up.

Which one is better? It depends on why you are using home plate.

Are you trying to avoid mid-chip solder balls, or are you trying to avoid tombstoning the ultra-small components. That is why you would use one or the other, in my humble opinion.

Phil
And by the way, there is a number of papers out there. If you look back through the different proceedings of both SMTAI and APEX you will find a number of papers.

You will even see some where, again for the same purposes Jim was discussing for some of the ultra-miniature passives and things like that, there are also experiments with what they call the roundese, which are basically radius edges as opposed to the straight-defined edges.

It is like everything else in this industry, for every paper or study done that is pro something you will find something that is "I'm against it!", the actual opposite. So as Jim said, understand why you are doing it in the first place and very carefully read up whatever you can.

But Jim gave the basics there, and that is what you want to follow. Do your homework, I guess.

Jim
One comment, Phil. Realizing that we are old you know whats and that we have been around forever. And there are young people out there who haven't.

If you weren't around during the transition from the miniaturization of chip components, to go down to 0402s and 0201s, the tombstoning issues were huge. People who had minimal amount of tombstones, all of a sudden you went to these small parts and you were getting a very, very high percentage of tombstoning.

Everybody was running around trying to figure out what was the best solution. And as my brother said, there were many of them proposed and different people had different opinions.

But if you weren't there it is difficult to understand the concern of trying to deal with all of these tombstones.

Phil
Good. Well, hopefully we answered the question in a non-ambiguous way. You just squandered another five minutes listening to Board Talk with Phil and Jim. Just remember, if you can't laugh at yourself, we certainly will. Whatever else you do, don't solder like my brother.

Jim
And don't solder like my brother.

Comments

Dec 13, 2024
I do the same thing as Steve O'Brien. It also prevents mid-chip solder balls and tombstoning, and works really, really well for cylindrical SMT glass MELF diodes. Otherwise, Most End up Laying on the Floor.
Richard Stadem, General Dynamics Mission Systems
May 21, 2021
When talking of inverted homeplate do you mean the homeplate is rotated to point the opposite direction or do you mean what is sometimes called a crown pad where the solder removed is pointing away from the center (so <] [> vs [< >]).
Tony Upton, Lonewolf PCB Ltd
May 21, 2021
I have used many of the home plate designs. Traditional, inverted, inverted radius, ETC. To me it is a "All Depends" scenario. Pad layout and solder paste can affect which works best. You just have to do some experiments and find out.
Alan Woodford, NeoTech
Nov 8, 2017
I always though the inverted home plate was shaped like a capital E with the triangle being a removed area of paste (similar to the Burgee or Swallowtail flag), where the inverted pointed area was placed under the component so the solder could flow up the side caps without pushing up from underneath.
Tony U., Schlumberger
Jun 29, 2017
For 10 years I used what was called the 'Inverse Radius Home Plate' design that was suggested by Fine Line Stencil. The purpose was to eliminate mid-chip solder balls. The solder paste was removed from the area under the component via the use of a gradual inverted radius that was located under and around the outer perimeter of the component. We never had problems keeping components where they were placed and solder balls were a thing of the past.
Timothy Bereman, BAE Systems
Jan 29, 2016
I agree with Steve, who commented prior to myself. It has been my understanding that an "Inverted Home Plate" Aperture is shaped like a little flag. The "outer" end of the aperture is a standard square shape, and the "inner" end of the aperture has two points that extend along the side of the component and a reverse point that will be located under the body of the component. This helps to both reduce the mid-chip solder ball (or bead), as well as helping to reduce tombstones on 0603 parts. (I personally use a 1:1 aperture on anything smaller than an 0603). This style of inverted Home Plate Aperture has served me well throughout the years.
Mark Hoch, Behr-Hella Thermocontrol Inc.
Mar 19, 2015
We use a variant on home plate apertures for chip components (jelly beans). We have the triangular ends cut into the aperture so it looks like a little flag. And we have the triangular ends facing towards the center of the component. What do you think of this arrangement?
Steve OBrien, CNS Precision, Australia
Submit A Comment
Comments are reviewed prior to posting. You must include your full name to have your comments posted. We will not post your email address.

Your Name


Your Company
Your E-mail


Your Country
Your Comments



Free Newsletter Subscription
Circuitnet is built for professionals who bear the responsibility of looking ahead, imagining the future, and preparing for it.

Insert Your Email Address

Sponsor
Advanced Interconnections Corp
Introducing our new Board to Board Connectors
These new Board to Board Connectors feature pitch sizes from 0.50 mm to 1.00 mm with multi-pitch and custom pitch designs available. Designed for long-life applications and robust handling.
Advanced Interconnections Corp
Precision Dispensing Solutions